High strength copper alloy is cast on the surface of 45# or GCr15 as the basic material of the bearing. This manufacturing process makes the copper and steel bonding surface achieve complete metallurgical bonding, which reduces the material cost and improves the bearing capacity. However, inlaying solid lubricant on the working face according to the working conditions greatly reduces the friction coefficient of the bearing and achieves the purpose of self-lubrication.

Contact Us > Download File

Technical Parameter


It can be seen from the metallographic diagram that there is mutual diffusion between the steel and copper alloy in the critical region, and the diffusion layer generated in the casting process is about 3μ-5μbetween the two materials to achieve complete metallurgical bonding and form a good bonding strength, which in any case exceeds the mechanical strength of the copper alloy itself.

The diffusion of steel and copper between each other provides excellent mechanical properties of this material, while the heat generated during the operation of the bearing can be transferred in time. The thin-walled copper alloy layer allows the double-layer material to have a similar coefficient of thermal expansion, so the 650GT material can be heat-treated as needed after casting, which means that this new material can ensure high accuracy and mechanical fit during use.

It combines the wear resistance of copper alloy with the high mechanical strength of steel.

· Different copper alloys can be cast according to the requirements of working conditions, including lead-copper alloys with low friction properties;

· Due to the different friction coefficients of the inner and outer layer materials, the bearing can be prevented from moving and rotating under high load and low speed conditions;

· It can be covered or inlaid with solid lubricant on the working surface as needed to achieve self-lubrication;

· Compared with pure copper sleeve, it has more cost advantages and saves resources;

· Can carry out post-processing, such as heat treatment of steel matrix, alloy layer machining, etc.;

· One or more layers of copper alloy casting can be performed on different or complex surfaces according to the design needs;

· Similar to the traditional copper sleeve in the use of characteristics, can be suitable for different temperatures under different lubrication conditions;

· Compared with pure copper sleeve, it has better mechanical bearing performance, especially impact strength


Material composition and properties table
Material grade450GT
400GT
450GT1
400GT1
450GT3
400GT3
450GT5
400GT5
Copper alloy compositionCuZn25Al5Mn4Fe3CuSn5Pb5Zn5CuSn12CuZn25Al5Mn4Fe3
Alloy layer hardness HB>210>70>95>250
Bonding strength of alloy layer Mpa>150>100>100>150
Maximum static load Mpa250150150250
Maximum dynamic load Mpa1006070120
Maximum linear velocity (dry) m/min15101015
Maximum PV valueN/mm2*m/min2006080200
Coefficient of thermal expansion 10-5/K1.2x10-5/℃1.2x10-5/℃1.2x10-5/℃1.2x10-5/℃
Service temperature℃-40~+300-40~+400-40~+400-40~+150
Permanent compressive deformation 300N/mm2<0.01mm<0.05mm<0.05mm<0.005mm